On this page
For a broader overview of test selection across chemistries, see capacity assessment.
Conditions that change the test method:
- Higher or lower discharge rates: Discharging faster than
C20reduces deliverable amp-hours due to Peukert's effect; apply the datasheet Peukert exponent (k) instead of comparing raw amp-hours directly to theC20nameplate. - Electrolyte temperature away from
25°C(77°F): Cold electrolyte increases internal resistance and lowers measured capacity; normalize results to25°C(77°F) before judging bank health. - Partial-depth field checks vs. full baseline tests: Full
100%DoD tests to1.75 V/cellverify end-of-life (<80%of ratedC20), whereas routine field checks can stop at50%usable DoD if the goal is verifying runtime margin without consuming a deep cycle. - 48.0V bus voltage ceiling: All test charging and recovery cycles on
12.0V,24.0V, and48.0Vbanks must remain strictly<=60V DC.
Core Specifications and Test Baselines
Verify exact cutoff voltages, Peukert exponent, and temperature coefficient on the battery datasheet or nameplate before starting a load test.
| Parameter | 12.0V Nominal Bank | 24.0V Nominal Bank | 48.0V Nominal Bank | Notes / Source |
|---|---|---|---|---|
| Cell count (2.0V/cell) | 6 cells | 12 cells | 24 cells | Standard lead-acid architecture |
| Standard test rate | C20 = Ah / 20 |
C20 = Ah / 20 |
C20 = Ah / 20 |
Constant-current 20 h rate |
Full-test cutoff (1.75 V/cell at C20) |
10.5 V |
21.0 V |
42.0 V |
Under load; stop immediately |
| Usable DoD baseline | 50% |
50% |
50% |
Typical cycling limit |
| Reference temperature | 25°C (77°F) |
25°C (77°F) |
25°C (77°F) |
Nameplate rating baseline |
| End-of-life threshold | <80% of rated C20 |
<80% of rated C20 |
<80% of rated C20 |
Corrected to 25°C (77°F) |
Governing Formulas (Plain Text)
20-Hour Test Current:
I_20 = C_20 / 20Example (illustrative): A12.0V,200 Ah(C20) bank requires a constant10 Atest load (200 Ah / 20 h = 10 A).Peukert Runtime & Effective Capacity (when
I_test != I_20):t = H * (C_20 / (I_test * H))^kC_effective = I_test * t = C_20 * (I_20 / I_test)^(k - 1)WhereH = 20hours,I_testis actual test current in amps, andkis the Peukert exponent (typically1.10–1.30for AGM/Gel and1.20–1.40for flooded; check the battery datasheet). Example (illustrative): Discharging that200 Ah(I_20 = 10 A) AGM bank (k = 1.15) at40 A:t = 20 * (200 / (40 * 20))^1.15 = 20 * (0.25)^1.15 = 4.06 hoursC_effective = 40 A * 4.06 h = 162.4 Ah(81.2%ofC20).Temperature Correction to
25°C(77°F):C_25C = C_measured / (1 + alpha * (T_C - 25))WhereT_Cis battery/electrolyte temperature in°Candalphais the datasheet temperature coefficient (commonly0.006 / °C, or0.6% / °C). Example (illustrative): Measuring176 Ahat5°C(41°F) withalpha = 0.006 / °C:C_25C = 176 / (1 + 0.006 * (5 - 25)) = 176 / 0.88 = 200 Ah.
Step-by-Step Capacity Test Procedure
1. Pre-Test Charge and Rest
- Fully charge the bank through bulk, absorption, and float stages according to the manufacturer's charging profile (keeping all system bus voltages
<=60V DC). - Disconnect all chargers and loads, then let the bank rest for 4 to 24 hours so surface charge dissipates and electrolyte temperature stabilizes.
- Measure and record resting open-circuit voltage (
OCV) and battery case or electrolyte temperature (°Cand°F). For flooded cells, verify electrolyte levels and specific gravity before starting.
2. Test Load and Measurement Setup
- Connect a calibrated constant-current DC load bank (or a stabilized inverter load at
120V/60HzAC in North America, or230V/50HzAC in UK/AU regions, monitored on the DC side with a calibrated shunt). - Size test leads for round-trip length (
2 x one-wayin feet or meters) to keep voltage drop<=3%and prevent premature low-voltage cutoff at the load terminals. - Measure voltage directly at the battery bank main terminals—not at the load bank or inverter input—using dedicated sense leads.
3. Controlled Discharge
- Start the discharge at
I_20(or a documented constant currentI_testwithin the datasheet Peukert curve). - Log terminal voltage, current (
A), cumulativeAh, and battery temperature at regular intervals (every30–60minutes atC20, or every10–15minutes at higher rates). - If testing a multi-string parallel bank or series-connected blocks (
12.0Vor6.0Vmonoblocks in24.0Vor48.0Vstrings), log individual monoblock voltages near the end of the discharge to catch a single weak block dragging down the bank. - Terminate the discharge immediately when the bank reaches the cutoff voltage (
10.5 Vfor12.0V,21.0 Vfor24.0V,42.0 Vfor48.0VatC20), or if any individual12.0Vmonoblock drops below10.5 V(5.25 Vfor6.0Vblocks).
4. Immediate Recharge
- Remove the load and begin recharging immediately—within minutes of test completion, never leaving the bank discharged overnight.
- Run a complete bulk and absorption cycle at the manufacturer-specified voltage and current limit (
<=60V DCon the bus). Verify that absorption current tapers to the datasheet tail-current threshold (~1–3%ofC20) before returning the bank to service.
Sign-Off Criteria
A lead-acid bank passes capacity assessment when all of the following are met:
- Corrected capacity
>=80%:C_25C(after Peukert and25°C/77°Fcorrection) is at least80%of the nameplateC20rating (or meets the site's minimum required runtime at design load above inverter/loadV_min). - Cell/monoblock balance: At
50%DoD and at test cutoff, individual12.0Vmonoblock voltages remain within0.2 Vof each other (0.1 Vfor6.0Vblocks), with no single block collapsing early. - Thermal stability: Battery temperature rise during a
C20discharge remains minimal (<=5°C/9°Fabove ambient) with no localized hot spots at inter-cell straps or terminals. - Full recovery: Post-test recharge reaches full absorption and expected resting
OCV(~12.6–12.8 Vper12.0Vunit after rest) without excessive gassing or thermal runaway.
Real Failure Modes
- Permanent Sulfation from Delayed Recharge: Leaving a lead-acid bank at
0%SoC after a capacity test allows soft lead sulfate to recrystallize into hard, non-conductive sulfate. Capacity drops permanently within hours to days. - False Fail from Uncorrected Cold Temperature: Testing a
200 Ahbank at0°C(32°F) yields roughly170 Ah(85%of25°Ccapacity) even on a healthy bank. Failing to apply temperature correction causes unnecessary battery replacement. - False Fail from Uncorrected High-Rate Peukert Loss: Running a
C20bank through a heavy inverter load (C4orC5) and comparing the rawAhcounter to theC20nameplate underreports true bank health by15–30%. - Voltage-Drop Premature Cutoff: Sensing voltage at an inverter or DC load connected through undersized or overly long test cables triggers the low-voltage cutoff while the battery terminals are still above
11.0 V(12.0Vbank), cutting the test short. - Reversed Weak Block in Series Strings: In
24.0Vor48.0Vseries strings, one degraded monoblock can hit0 Vor reverse polarity before the total bank string reaches21.0 Vor42.0 V, permanently destroying that block unless per-block voltages are monitored.